Stress Relieving Temperature for Steel Fabrications: A Guide

Advance Heating Systems
1 day ago
5 min read

Welding, heavy machining and cold forming leave stresses locked inside steel parts. Those stresses can cause distortion during later machining, and they raise the risk of brittle fracture and stress corrosion cracking in service. Stress relieving, often called post-weld heat treatment (PWHT) for welded parts, reduces them.

This guide explains the temperatures, soak times and furnace practice involved. It is based mainly on TWI's published guidance. For code work, always follow the specific code and your approved procedure.

Key takeaways

  • PWHT reduces residual stress and improves toughness, lowering the risk of brittle fracture and stress corrosion cracking. TWI notes it gives little fatigue benefit.

  • For carbon steel, typical PWHT ranges are about 550–620°C, depending on the code.

  • Cr-Mo steels need higher temperatures, up to about 750°C for 5Cr-Mo.

  • A common rule is a soak of about 1 hour per 25 mm of thickness.

  • Heating and cooling rates above about 350–400°C are controlled by codes. Too fast causes distortion or cracking.

  • A furnace is the best method, with load thermocouples and no direct flame contact.

Why stress relieve?

TWI explains that PWHT lowers residual stresses and improves toughness. That reduces the risk of brittle fracture and stress corrosion cracking. It does little for fatigue life (TWI Job Knowledge 115).

Typical work that needs it:

  • pressure vessels and boiler parts;

  • heavy fabrications that will be machined after welding, to avoid distortion;

  • hydro and power plant components;

  • some castings and forgings.

Stress relieving temperatures by steel type

TWI compares the temperature requirements of three major pressure vessel codes:

Steel

EN 13445 range

ASME VIII minimum hold

PD 5500 range

Carbon steel

550–600°C

593°C

580–620°C

C-½Mo

550–620°C

593°C

630–670°C

1Cr-½Mo

630–680°C

593°C

630–700°C

2¼Cr-Mo

670–720°C

677°C

630–750°C

5Cr-Mo

700–750°C

677°C

710–750°C

Source: TWI.

Notice that the codes do not agree exactly. Use the code your job is built to, and your approved procedure, not a general table. For steels not in this table, such as tool steels, spring steels and stainless steels, ask your material supplier.

How long to soak

TWI gives a rule of thumb of about 1 hour per 25 mm of thickness.

Section thickness

Approx. soak at temperature

25 mm

1 hour

50 mm

2 hours

75 mm

3 hours

100 mm

4 hours

Codes may set their own minimum times. Time the soak from when the load reaches temperature, not the furnace air.

When is PWHT mandatory?

TWI notes that PWHT becomes mandatory above certain thicknesses:

  • above 19 mm under ASME VIII;

  • above 35 mm under EN 13445 and PD 5500.

Thresholds and exemptions depend on material and code, so check your specific code.

Heating and cooling rates

TWI notes that codes control heating and cooling rates above about 350–400°C. If you heat or cool too fast, thick and thin sections reach different temperatures, causing new stresses, distortion or cracking.

In practice:

  • the code-controlled part of the cycle starts above about 350–400°C, so check what your code allows for loading temperature;

  • above that range, ramp at the rate your code allows;

  • soak;

  • cool at a controlled rate down to about 350–400°C, then cool in still air if the code allows.

A programmable ramp-soak controller makes this repeatable, and a recorder gives you the time-temperature chart many inspectors require.

Furnace practice that gets it right

TWI recommends a furnace as the best way to stress relieve, using bogie-loaded or top-hat furnaces for large work. Key points:

Keep flames off the work

Gas flames must not touch the part or the thermocouples. Direct impingement causes local overheating and false readings. Burner placement and baffling matter.

Check fuel sulphur

TWI advises checking the sulphur content of the fuel used in fuel-fired furnaces. Ask your fuel supplier for this figure before running code work.

Use load thermocouples

Zone control with thermocouples on the load is preferred over air temperature alone. Place them on the thickest and thinnest sections.

Support the work

Support components on trestles so they do not sag at temperature.

Get uniform temperature

Multi-zone heating and roof circulation fans even out temperature in large furnaces.

What a stress relieving furnace looks like

For large fabrications, a bogie hearth furnace is the usual choice. The load sits on a wheeled car (bogie) that rolls out for loading by crane.

As an example, we built a bogie-type stress-annealing furnace for an export customer in Nepal in 2025 with:

  • inside size of 7,000 × 1,800 × 1,200 mm;

  • maximum temperature 1,000°C, operating 500–950°C, ±5°C;

  • three heating zones with automatic-ignition burners;

  • three SS-310 roof circulation fans with water-cooled assemblies;

  • 250 mm ceramic-fibre insulation;

  • two bogies, so one can be loaded while the other is in the furnace;

  • outer wall temperature designed to be no more than about 25°C above ambient.

For smaller parts, a box or chamber furnace, or a lower-temperature stress relieving oven, may be enough. See our stress relieving bogie hearth furnace and the general bogie hearth furnace page.

Electric or gas?

Factor

Electric

Gas (PNG / LPG)

Temperature uniformity

Very good with zoned heaters

Good with correct burners and fans

Large furnaces

Needs a high connected load

Easier to deliver large heat input

Flame contact risk

None

Burner design must prevent it

Emissions

None at site

Clean fuel; check local rules

Electric furnaces at these temperatures use resistance alloys with plenty of margin. Kanthal rates NiCr 80/20 to 1,200°C and Kanthal A-1 to 1,400°C maximum element temperature in air, well above PWHT temperatures.

Frequently asked questions

What is the stress relieving temperature for mild steel? For carbon steel, TWI lists 550–600°C under EN 13445, a 593°C minimum hold under ASME VIII, and 580–620°C under PD 5500. Follow your code.

How long should I soak for stress relieving? A common rule is about 1 hour per 25 mm of thickness, timed from when the load reaches temperature. Codes may set minimums.

When is PWHT mandatory? TWI notes thresholds of above 19 mm under ASME VIII and above 35 mm under EN 13445 / PD 5500. Check your code for material-specific rules.

Does stress relieving improve fatigue life? TWI says PWHT gives little fatigue benefit. Its main benefits are lower residual stress and better toughness.

Can I stress relieve in a gas-fired furnace? Yes, provided flames do not touch the work or thermocouples, the fuel's sulphur content is acceptable, and temperature control is good.

Get a stress relieving furnace quotation

Tell us your largest job size and weight, steel types, temperatures and the code you work to. We will propose a bogie, box or pit design with suitable controls and recording. Heavy fabrication and forging units can also visit our steel, forging and casting industries page.

Call +91 98105 20120 or email enquiry@ahs-in.com. Advance Heating Systems, Hastsal Industrial Area, New Delhi 110059.

Comments


bottom of page