How to Bake and Redry Welding Electrodes: E7018, E6013 and More
Moisture in an electrode coating turns into hydrogen in the weld. On structural, pressure and boiler work, that hydrogen can cause cracking hours or days after welding. Baking and holding ovens keep moisture out of the coating, but only if you use the right temperature, time and loading.
This guide collects the published redrying guidance from electrode makers in one place and adds practical points from our work. Advance Heating Systems has built electrode baking ovens in Delhi since 1991. Electrode baking ovens are one of the two largest product lines in our archive of 3,700+ quotations and project documents since 2002.
Key takeaways
Low-hydrogen E7018/E7028 (not wet): redry at 340–400°C (650–750°F) for 1 hour, per Lincoln Electric.
Higher-strength E8018 to E11018: 370–430°C (700–800°F), and no more than three one-hour redries.
Rutile and similar types (E6012, E6013, E7014): redry at 200–260°C (400–500°F) for 30–45 minutes.
Cellulosic E6010/E6011: do not rebake. Hold at only 40–50°C.
Holding ovens for opened low-hydrogen stock run at about 120–150°C.
Load shallow. A heavy charge can take hours longer to reach temperature at the core than the oven display suggests.
Always check the datasheet of your electrode brand first. It overrides any general table.
Why electrodes need baking at all
Electrode coatings pick up moisture from the air once a can or box is opened. ESAB says low-hydrogen electrodes leave the factory with about 0.1–0.4% moisture in the coating. Cellulosic electrodes are deliberately made with about 4–6% moisture, because they need it to weld properly.
That is why one oven setting cannot suit every electrode. Overheating a cellulosic rod ruins it. Underheating a low-hydrogen rod leaves the moisture in. ESAB also advises against storing cellulosic and low-hydrogen electrodes in the same oven.
Redrying temperatures by electrode type
The table below summarises Lincoln Electric's published storing and redrying guidance. Use it as a starting point, then confirm with your supplier's datasheet.
Electrode group | Examples | Redry temperature | Redry time | Holding / storage |
Low-hydrogen, carbon steel | E7018, E7028 | 340–400°C (650–750°F) | 1 hour | 120–150°C (250–300°F) |
Low-hydrogen, wet | E7018 that got wet | Pre-dry 80–105°C (180–220°F) for 1–2 h, then the redry above | 1–2 h + 1 h | 120–150°C |
Low-hydrogen, higher strength | E8018 to E11018 | 370–430°C (700–800°F) | 1 hour, max three redries | 120–150°C |
"Fast Fill" types | E6012, E6013, E7014 | 200–260°C (400–500°F) | 30–45 minutes | Per datasheet |
Cellulosic "Fast Freeze" | E6010, E6011 | Rebaking not recommended | — | 40–50°C (100–120°F) |
Wet electrodes need a two-step bake
If low-hydrogen electrodes have actually got wet, do not put them straight into a hot oven at 350°C. Lincoln recommends a pre-dry at 80–105°C for 1–2 hours first, then the normal final redry. Going straight to high heat can crack or blister the coating.
Limit the number of redries
Repeated redrying weakens the coating. Lincoln limits E8018 to E11018 electrodes to three one-hour redries. Keep a simple log by batch so your stores team knows how many times a lot has been baked.
Holding ovens: the step most plants skip
A baking oven drives moisture out. A holding oven keeps it out until the welder uses the rod.
Lincoln gives 120–150°C (250–300°F) for holding opened low-hydrogen electrodes.
ESAB says most manufacturers recommend 225–300°F (about 107–150°C) for low-hydrogen holding.
ESAB's baking procedure says to hold baked electrodes at about 150°C, and keep portable quivers at the work site at 70–130°C.
Lincoln also says standard EXX18 electrodes should be issued to welders twice per shift. Moisture-resistant "R" types allow up to 9 hours of exposure. Your welding procedure or project code may set its own exposure limits, so check the specification you are working to.
Loading: why oven temperature is not electrode temperature
This is where many plants go wrong. The oven display shows air temperature. The electrode core lags behind, because the flux coating insulates it.
TWI reports a trial with the oven set at 250°C:
20 kg charge: the oven took about 45 minutes to recover after loading. The electrode centres reached 230°C about 50 minutes after that.
80 kg charge: the oven took about 2.5 hours to recover. The electrode centres reached only 200°C after about 6 hours.
So if you load 80 kg and start a one-hour timer when the door closes, the electrodes may never reach the redry temperature. See TWI's FAQ on baking low-hydrogen electrodes.
Practical loading rules
ESAB's step-by-step baking procedure gives clear shop-floor rules (ESAB baking procedure):
Preheat the oven to at least 100°C before loading.
Keep the moisture vent open during baking.
Load no more than four layers per rack.
Do not mix diameters on one rack.
Start the timer only once the load is at baking temperature.
In our ovens we fit an exhaust blower on a cyclic timer to clear moisture-laden air, and a multi-point recorder so supervisors can see more than one location in the chamber.
What to do after a power cut
Power cuts are common in many Indian industrial areas, and welding forums often discuss what to do after a temperature drop. There is no single published rule for every case. A sensible approach:
Treat the oven as "out of control" for the duration of the dip.
If the electrodes were in a holding oven and the dip was short, bring the oven back to holding temperature and check your project procedure.
If you are unsure how long they were exposed, or if the oven fell to room temperature, redry them per the table above. Count it as one of the allowed redries.
Record the event against the batch.
A recorder with data logging makes this much easier, because you can see exactly how long the dip lasted. For plants with frequent outages or gas shortages, a dual-fuel oven that can switch between electric and LPG/PNG heating keeps production moving. See our dual-fuel electrode baking oven.
Baking oven vs holding oven: do you need both?
Feature | Baking / redrying oven | Holding oven |
Typical range | Up to 350–450°C | About 100–150°C |
Purpose | Remove absorbed moisture | Stop moisture pick-up |
Batch size | Larger charges, timed cycles | Daily issue stock |
Location | Stores / central | Near the welding bay |
Most fabricators with low-hydrogen work need both. A high-temperature oven can hold at 150°C, but then it is tied up and cannot redry the next batch. Our electrode holding and testing oven is sized for the holding role. For production and redrying, see our electrode baking oven range. Electrode manufacturers can read more on our welding electrode industry page.
Frequently asked questions
At what temperature should E7018 electrodes be baked? Lincoln Electric gives 340–400°C (650–750°F) for one hour for E7018 that has been exposed for less than a week and is not wet. Then hold at 120–150°C. Always check your brand's datasheet.
Can E6013 electrodes be baked? Yes. Lincoln lists E6012, E6013 and E7014 for redrying at 200–260°C (400–500°F) for 30–45 minutes. That is much lower than for low-hydrogen types.
Should E6010 electrodes be rebaked? No. Lincoln does not recommend rebaking cellulosic E6010/E6011 electrodes. They need their moisture to weld properly. Store them at 40–50°C.
How many times can low-hydrogen electrodes be redried? Lincoln limits E8018 to E11018 electrodes to three one-hour redries. For other grades, follow the manufacturer's datasheet and keep a batch log.
Why do my electrodes still give porosity after baking? Often the oven was overloaded or the timer started too early. TWI found an 80 kg charge took about 6 hours for the electrode cores to reach 200°C at a 250°C setting. Load in shallow layers and start timing at temperature.
Get the right electrode oven for your plant
AHS designs batch, continuous and dual-fuel electrode baking ovens, and holding ovens, for fabricators and electrode manufacturers in India and abroad. Tell us your electrode types, kg per shift and power or gas supply, and we will recommend a size and heating method.
Call +91 98105 20120 or email enquiry@ahs-in.com for a quotation. Advance Heating Systems, Hastsal Industrial Area, New Delhi 110059.



Comments