top of page

Annealing Temperature for Aluminium Circles and Sheets

Advance Heating Systems
1 day ago
5 min read

Cold rolling makes aluminium sheet hard. If you try to deep-draw a hard circle into a pressure cooker body or kadhai, it splits or wrinkles. Annealing softens the metal again so it can be drawn.

Aluminium circle annealing is the largest single product family in Advance Heating Systems' records, with more than 550 documents from 2004 to 2026. This guide explains the temperatures involved, why results vary from batch to batch, and what to look for in an annealing oven.

Key takeaways

  • Recovery (partial softening) starts at about 90–120°C and continues up to about 230°C.

  • Full softening by recrystallisation of heavily cold-worked commercial alloys happens after several hours at 340–410°C, per Total Materia.

  • Full annealing gives O temper, the soft, highly formable condition used for deep drawing utensils.

  • Partial annealing gives intermediate H22–H28 tempers.

  • The metal temperature in the middle of the stack matters, not the air temperature at the controller.

  • Good air circulation, enough soak time and accurate control matter more than a high setpoint.

  • Confirm the exact cycle for your alloy and temper with your metal supplier.

What happens when you anneal aluminium

Annealing works in two stages.

Recovery

According to Total Materia's guide to annealing aluminium, recovery begins at about 90–120°C. Internal stresses relax and the metal softens slightly. Softening by recovery alone continues up to about 230°C. This is not enough to give a fully soft circle for deep drawing.

Recrystallisation

At higher temperatures, new strain-free grains form and replace the deformed grains from rolling. Total Materia states that heavily cold-worked commercial alloys recrystallise after several hours at 340–410°C (650–775°F). This is full annealing and gives the O temper.

If you stop between recovery and full recrystallisation, you get a partially annealed temper, designated H22 to H28. These are harder than O temper but softer than as-rolled.

For a deeper technical reference, see NIST's Heat Treating of Aluminum Alloys.

Why O temper matters for utensil makers

O temper is the soft, highly formable condition that suits deep drawing of pots, pans, pressure cookers and similar shapes. If circles crack at the bottom radius or show uneven earing, the first thing to check is whether the whole charge actually reached full annealing.

Temper

How you get it

Typical use

H1x (as rolled)

Cold rolling, no anneal

Flat parts, light forming

H22–H28

Partial anneal

Moderate forming, some strength retained

O (fully annealed)

Full recrystallisation anneal

Deep drawing: utensils, cookware

Reading the temperature range correctly

The 340–410°C figure is a range for metal temperature, held for several hours. Three things often go wrong on the shop floor.

1. Air temperature is not metal temperature

The controller reads air near its thermocouple. Circles stacked tightly in the middle of a 500 kg charge heat much more slowly. If you start the soak timer when the air reaches setpoint, the centre may never get there.

Fix: use a load thermocouple placed in the middle of the stack, at least during trials, and start soaking once that reading reaches setpoint.

2. Uneven airflow gives hard and soft circles in the same batch

Without strong circulation, the top and outer circles anneal while the inner ones stay hard. Side circulation fans and a well-designed air path are essential.

3. Different alloys and reductions behave differently

The amount of cold work, the alloy and the gauge all change the time and temperature needed. Heavily reduced sheet recrystallises more readily than lightly reduced sheet. Ask your sheet or coil supplier for their recommended annealing cycle, and do a trial with a load thermocouple to confirm it.

A practical approach to setting your cycle

  1. Get the supplier's recommended cycle for your alloy and temper.

  2. Load a trial charge with thermocouples in the centre, top and edge of the stack.

  3. Ramp up and note when the slowest thermocouple reaches setpoint.

  4. Soak from that point, not from when the air reached setpoint.

  5. Cool as recommended, then test hardness or do a trial draw from circles taken from different positions.

  6. Record the cycle and lock it into the controller's soak timer.

What to look for in an annealing oven

Most utensil and circle makers in India use trolley-type batch ovens. Our standard designs share these features:

Feature

AHS typical design

Charge

500 kg per charge is our most common size; larger ovens up to about 4,000 kg

Maximum temperature

500–550°C (some to 800°C)

Operating range

100–500°C

Loading

Trolley; two trolleys on larger ovens so one loads while the other heats

Heating

LPG/PNG burner in a separate top firing chamber, electric heaters (54–90 kW, 60 kW most common), or wood-pellet burner

Insulation

125–150 mm ceramic fibre plus mineral wool

Firing chamber

Stainless steel

Controls

Digital PID with soaking timer

Gas safety

Flame-failure gas cut-off with audio-visual alarm

See our circle aluminium annealing oven for details, and our trolley oven range for other batch sizes.

Fuel choice and cost per batch

Energy is now the biggest worry for many circle and utensil units. The aluminium extrusion industry body ALEMAI reported in September 2026 that energy costs had risen about 30% since the post-Hormuz crisis. Before choosing a fuel, compare cost per batch, not cost per hour. Our electric vs PNG vs LPG running cost guide shows how to do the maths.

We have also quoted annealing ovens with a wood-pellet burner and an electric switch-over option. If your plant is in Delhi NCR, check that the fuel is permitted under the current CAQM approved fuel list before choosing it.

Frequently asked questions

What is the annealing temperature for aluminium sheet? For full annealing (O temper) of heavily cold-worked commercial alloys, Total Materia gives several hours at 340–410°C. The exact cycle depends on alloy, gauge and prior cold work, so confirm it with your sheet supplier.

Why do my aluminium circles crack during deep drawing? Common causes are incomplete annealing (the centre of the stack did not reach temperature or was not soaked long enough), uneven air circulation in the oven, or a temper unsuitable for the draw depth. Check with load thermocouples.

What is the difference between O temper and H24? O is fully annealed and fully soft. H22–H28 are partially annealed tempers that keep some of the rolled strength. Deep-drawn utensils normally need O temper.

How long should the soak be? Long enough for the slowest part of the charge to reach temperature and recrystallise. Total Materia refers to "several hours" in the 340–410°C range. Time your soak from when the load thermocouple, not the air, reaches setpoint.

Can one oven anneal both circles and coils? Often yes, with suitable trolleys or charge carriers. Coils are dense and heat slowly, so cycle times are longer. Tell us your charge sizes when you ask for a quote.

Talk to AHS about your annealing oven

We have built annealing ovens for circle, sheet and utensil makers across India and for export since 1991. Send us your charge weight, circle sizes and fuel options, and we will propose a design.

Call +91 98105 20120 or email enquiry@ahs-in.com. Advance Heating Systems, Hastsal Industrial Area, New Delhi 110059. See also our aluminium utensils industry page.

Comments